Match Your Nozzle to the Resin and the Mold

Nozzle selection is often reduced to "whatever fits". Three dimensions decide whether the process runs properly.
Orifice diameter
The orifice sets the shear rate at the gate and the pressure drop. Too small and you lose pressure and generate heat; too large and you cannot control freeze-off, so you get drool and stringing.
- Small parts, low shot weight: 2 - 4 mm, subject to the resin's shear sensitivity
- General parts: 4 - 6 mm
- Large parts and high flow rates: 6 - 10 mm
- Glass filled resins: add 1 - 2 mm over the unfilled recommendation to reduce wear
- Shear sensitive resins (PVC): generous orifice, no sharp entry
Tip radius and seat
The tip radius must match the sprue bushing radius exactly. A mismatch produces a ring of flash at the interface, which cools and blocks the next shot, or a gap that leaks melt across the mold face. Check the radius with a radius gauge rather than by eye, and confirm the contact is a line contact, not a face contact.
Body length
Too short and the nozzle cannot reach the sprue bushing; too long and it overhangs, unsupported, and bends. Measure from the barrel face to the sprue bushing seat with the mold clamped, then allow for thermal expansion at operating temperature.
Symptoms and their nozzle cause
- Stringing: orifice too large, or tip temperature too high
- Cold slug in the sprue: nozzle too cold, or tip contact too long
- Short shots at the same pressure: orifice too small for the fill rate
- Flash ring at the sprue: radius mismatch
- Drool between shots: worn seat, or decompression insufficient
See nozzle bodies and tips and nozzle band heaters.
Related products