แนวปฏิบัติพัจจิ้งคอมพาวด์สำหรับเปลี่ยนสี

Purging is usually done by feel, which is why it consumes more material than it needs to and still leaves streaks in the first parts.
The procedure that works
- Purge at the outgoing resin's temperature, not the incoming one. The material you are removing has to be soft enough to move.
- Empty the hopper and run the screw until the shot starts to starve.
- Add purging compound at roughly the barrel capacity, no more. Extra compound does not clean better; it just costs more.
- Low back pressure, moderate screw speed. High speed smears the compound rather than scrubbing the flights.
- Allow dwell for chemical grades — 5 to 15 minutes with the screw forward.
- Purge with full strokes until the slug is uniform. Look at the slug, not just the color of the surface.
- Introduce the new resin and purge one more barrel capacity before production.
Judging cleanliness
A purge slug that looks clean on the outside can still carry a stripe of the old color inside. Cut the slug lengthways. If the core is uniform, the barrel is clean; if there is a spiral stripe, keep going. This single check prevents most first-shot rejections.
Reducing purging waste
- Plan color changes in sequence, light to dark, so one purge serves two changes
- Keep a dedicated purge grade for hot runners; standard compound leaves residue in drops
- Record the actual quantity used per change and set a target; most shops can halve it
- Do not use production resin as a purge unless the colors are compatible — it is the most expensive option
- For black-to-natural changes, a mechanical compound followed by a small chemical dose works better than either alone
See the purging compound range and cleaners.