Troubleshooting Black Specks and Burn Marks

NEWS

Black specks are rarely random. They come from a place where resin sits still and gets hot, and finding that place is a process of elimination rather than guesswork.

First, decide whether it is degradation or contamination

Degradation specks are soft, smeary and often surrounded by a brown halo. Contamination specks are hard, angular and unrelated to the surrounding color — often the previous resin, a regrind fragment, or dirt from the material handling system. Cut a part open and look at the specks under a magnifier before changing any settings.

Where degradation specks come from

  • Excessive residence time: shot size below 25% of barrel capacity, or a barrel too large for the mold
  • Hot runner dead spots: a drop with a thermocouple reading the manifold, running hotter than it reports
  • Worn screw flights or a leaking check ring: resin holed up in the flight root and cooked between shots
  • Nozzle and tip stagnation: a tip with a sharp internal corner, or a nozzle that is too long for the mold
  • Temperature too high for the resin: check the actual melt temperature with a needle probe, not the setpoint

Where contamination specks come from

  • Open gaylords and unsealed hoppers
  • Regrind mixed with a different color or a different resin
  • Dust from cardboard, or from a granulator running dry
  • Hose and loader interiors shedding material

Elimination order

Purge properly and shoot a slug — if specks appear in the slug, the source is upstream of the nozzle. If the slug is clean but parts are not, the source is the hot runner or the mold. Raise all zones by 10 °C; if specks get worse, you have degradation and the zone is suspect. Reduce melt temperature and increase screw speed slightly to shorten residence time. If the problem persists, pull the screw and inspect the flights and check ring.

See purging compounds, gaylord covers and barrels.