Dongguan International Technology Transfer Center, 124 Dongbao Road, Dongcheng District, Dongguan, China
Request a quote
Centron Engineering News & Articles

How to Diagnose Screw and Barrel Wear

NEWS

Screw and barrel wear is gradual, which is why it is usually blamed on something else first: the mold, the resin, the controller. By the time output has dropped enough to be obvious, the clearance is often two or three times the original value.

Five signs that point at the injection unit

  1. Falling shot weight at the same setpoints. If the cushion is shrinking and you are adding stroke to compensate, melt is leaking back over the flights.
  2. Longer recovery time. A worn screw conveys less per revolution, so the screw has to turn longer to build the same shot.
  3. Inconsistent part weight. Variation above 0.5% on a stable process usually means the non-return valve or the flights are worn.
  4. Black specks or streaks that survive purging. Resin is holed up in a worn flight root or behind a damaged check ring.
  5. Visible wear on inspection. Pull the screw and look at the flight OD, the flight root and the check ring seat.

Measuring clearance in the workshop

You do not need a metrology lab. Measure the flight OD with a micrometer at the feed, compression and metering sections, then measure the barrel bore with an inside micrometer or a bore gauge at the same positions. Diametral clearance for a typical nitrided screw and barrel starts around 0.10 - 0.15 mm new. Once it passes roughly 0.35 - 0.40 mm, recovery and shot repeatability will not come back through tuning.

Also check the check ring. A ring that rattles freely on its seat, or shows a rounded sealing face, is leaking. Replacing a ring and seat on an otherwise healthy screw is a fraction of the cost of a new injection unit.

Repair or replace

  • Recondition when wear is even, the barrel bore is within tolerance and only the flights need rebuilding
  • Replace both when the barrel is barrel-shaped or scored — a new screw in a worn barrel wears out fast
  • Upgrade the material if the resin is glass or mineral filled; a bimetallic barrel and screw will outlast nitrided components several times over

Keep the measurement record with the machine. Wear trends matter more than a single reading: a screw that lost 0.1 mm in six months has a different problem from one that lost it over five years.

Related reading: injection molding screws and barrels.